EPDM is the compound for water, steam and weather, and it is the one material on this list that can sit outdoors for twenty years without cracking. Where a joint carries hot water, a wash-down line, a cooling circuit or an outside seal, EPDM is usually both the cheapest answer and the longest lived one.
Its weakness is equally clear. EPDM and mineral oil do not coexist: a single contact with grease swells the ring until it will not seat, and the swelling is not reversible. That single fact decides most EPDM enquiries before any other property is discussed.
What EPDM Is
EPDM is a terpolymer of ethylene, propylene and a diene monomer. The saturated backbone is why it resists ozone, ultraviolet light and heat ageing so well, and why it has no unsaturated chain for oil to attack, which is also why it has no oil resistance at all. Ethylene content sets the balance: more ethylene gives higher tensile strength and better extrusion resistance, less keeps the compound flexible at low temperature. Peroxide cured grades hold up to 150 °C and hold compression set better than sulphur cured ones, at a higher price.
Properties At A Glance
The figures below are typical for a 70 Shore A compound of this class, which is the hardness most of our stock and most drawings call for. A 90 Shore A version of the same polymer will sit at the top of the hardness range and at the bottom of the temperature range.
| Property | Typical value | What it means |
|---|---|---|
| Hardness | 40 to 90 Shore A | 70 for general service; 80 to 90 for steam and pressure |
| Temperature range | −50 to +150 °C | Sulphur cured to 120 °C, peroxide cured to 150 °C |
| Colour | Black | White and grey for food and drinking water grades |
| Tensile strength | 8 to 15 MPa | Lower than NBR; adequate for static sealing |
| Compression set | Good | Peroxide cure is markedly better at 120 °C and above |
| Ozone and weather | Excellent | No cracking in outdoor service |
| Relative cost | Low to moderate | Close to NBR, well below FKM |
Where It Works
- Hot water, cold water, wash-down lines and cooling circuits
- Steam up to about 150 °C with a peroxide cured grade
- Outdoor and ozone exposed joints, including roof and façade work
- Dilute acids, bases and phosphate ester hydraulic fluids
- Drinking water, with WRAS or NSF 61 approved grades
Where It Fails
- Mineral oil, grease and every petroleum based lubricant, which swell it badly
- Aromatic and aliphatic hydrocarbon solvents
- Concentrated oxidising acids
- Petrol and diesel, where swelling is fast and permanent
- Applications that need high tensile strength or tear resistance, where NBR is better
Resistance To Common Media
Ratings are for the compound class at room temperature unless the note says otherwise, and they describe swelling, hardening and loss of strength together rather than one figure. A compound that swells 20 percent has already changed its squeeze.
| Medium | Rating | In practice |
|---|---|---|
| Hot water | Excellent | The reference application; peroxide cure for 130 °C and above |
| Steam | Good | To about 150 °C; decompression of the compound matters at the top of the range |
| Mineral oil and grease | Poor | Severe swell, often 50 percent or more |
| Petrol and diesel | Poor | Not a fuel compound |
| Dilute acids and bases | Good | Better than NBR on both sides of the pH scale |
| Phosphate ester hydraulic fluid | Good | One of the few elastomers that suits it |
| Ozone and weather | Excellent | The reason it is used outdoors |
| Ketones and esters | Fair | Some swelling; test where the duty is continuous |
Compounds We Quote
We quote EPDM from 40 to 90 Shore A, sulphur cured for general water service and peroxide cured for steam, hot water above 120 °C and low compression set. Drinking water grades to WRAS and NSF 61 and food grades to FDA 21 CFR 177.2600 are available on request, and those approvals are quoted as certificates rather than claimed on the page.
For a steam joint the cure system is worth as much attention as the polymer. A sulphur cured EPDM that reads well on a data sheet will take a set in a 140 °C steam line within a season, while the peroxide grade in the same groove will not.
Sizes And Standards
Choosing between compounds rather than specifying one? The O-ring material comparison puts all five side by side at 70 Shore A, with the temperature range and the media each one cannot take.
The size is a separate decision from the compound, and it is the one buyers most often get wrong. The four standard lists are on their own pages, each with a lookup that takes either the code or a pair of measured dimensions: AS568 (inch dash numbers), ISO 3601 (Class A and Class B metric), JIS B 2401 (P, G, S, SS and V series) and BS 1806 (British imperial numbers). If the drawing gives a size outside those lists, or a cord that is not standard, we mould to drawing.
What To Send With An Enquiry
- The size or dash number, and the standard it comes from
- Whether the duty is water, steam, or a chemical, and at what temperature
- The approval needed: WRAS, NSF 61, FDA, or none
- Hardness, and the pressure if the joint sees more than a few bar
- Whether the seal is exposed to oil anywhere in the plant, including assembly grease
Can EPDM O-rings be used with oil?
No. Mineral oil, grease and petroleum based lubricants swell EPDM severely and the change is permanent. If the joint is assembled with grease, either use a silicone grease approved for EPDM or fit NBR instead.
What is the temperature limit for EPDM?
150 °C for a peroxide cured compound in continuous service, and about 120 °C for a sulphur cured one. Short excursions above that are tolerable, but the compression set that follows is what causes the leak.
Is EPDM suitable for drinking water?
Yes, in an approved grade. We supply WRAS and NSF 61 compounds on request with the certificate, which is what a water utility will ask for rather than a general statement of suitability.
Why did my EPDM ring fail in steam?
Usually a sulphur cured compound in a joint above 130 °C, or rapid decompression pulling the ring apart. Both are cure and formulation questions rather than a fault in the polymer, and both are quoted as a different compound rather than a different size.