FKM, sold as Viton and as a dozen other trade names, is the compound for heat, fuel and aggressive chemistry. It is the only material on this matrix that holds a seal at 200 °C and still resists aromatic fuel, which is why it appears wherever the duty is an engine, a solvent line or a hot hydraulic system.
The price is the first thing a buyer notices and the low temperature limit is the second. FKM stiffens below about −20 °C, and a standard grade asked to seal at −30 °C will leak on start-up even though it was perfect in the test cell. Both facts belong in the enquiry, not in the post mortem.
What FKM Is
FKM is a fluoroelastomer: a copolymer of vinylidene fluoride with hexafluoropropylene, and sometimes tetrafluoroethylene. The fluorine content, typically 66 to 70 percent, is what buys the heat and chemical resistance, and the monomer ratio is what sets the low temperature behaviour. A standard grade stops flexing near −20 °C; a low temperature grade with a different monomer balance reaches −40 °C at some cost in fluid resistance, which is the trade a cold climate buyer has to make explicitly.
Properties At A Glance
The figures below are typical for a 70 Shore A compound of this class, which is the hardness most of our stock and most drawings call for. A 90 Shore A version of the same polymer will sit at the top of the hardness range and at the bottom of the temperature range.
| Property | Typical value | What it means |
|---|---|---|
| Hardness | 50 to 90 Shore A | 70 and 75 are the common drawing figures |
| Temperature range | −20 to +200 °C | Low temperature grades to −40 °C; short excursions to 230 °C |
| Colour | Black, brown, green | Green is often a Viton GFLT marker rather than a specification |
| Tensile strength | 10 to 16 MPa | Retained well at temperature, which is the point of FKM |
| Compression set | Excellent | The best of the five at 150 °C and above |
| Fluid resistance | Excellent | Aromatic fuels, solvents, acids and hydraulic fluids |
| Relative cost | High | Three to five times an NBR compound of the same size |
Where It Works
- Petrol, diesel, biodiesel blends and aromatic fuels
- Aromatic and chlorinated solvents, and most acids
- Hot hydraulic and transmission oil at 150 °C and above
- Vacuum service where outgassing has to stay low
- Engine and compressor seals, where the joint cycles hot and dry
Where It Fails
- Hot water and steam above about 100 °C, which attack the polymer rather than swell it
- Low temperature start-up below −20 °C with a standard grade
- Amines, ammonia and strong bases
- Ketones, esters and low molecular weight ethers
- Cost sensitive static joints that NBR would seal for a tenth of the price
Resistance To Common Media
Ratings are for the compound class at room temperature unless the note says otherwise, and they describe swelling, hardening and loss of strength together rather than one figure. A compound that swells 20 percent has already changed its squeeze.
| Medium | Rating | In practice |
|---|---|---|
| Petrol and aromatic fuel | Excellent | The reference application |
| Diesel and biodiesel | Excellent | Biodiesel blends above B20 are worth testing |
| Mineral and synthetic oil at 150 °C | Excellent | Where NBR has already failed |
| Aromatic and chlorinated solvents | Good | Depends on the specific solvent; send the name |
| Hot water and steam | Poor | Degrades rather than swells; EPDM is the answer |
| Dilute and concentrated acids | Good | Better than any other compound on this list |
| Amines and ammonia | Poor | A known FKM limit |
| Low temperature below −20 °C | Fair | Only with a low temperature grade, and even then check the test |
Compounds We Quote
We quote FKM from 50 to 90 Shore A in standard and low temperature grades, with peroxide curable and bisphenol cured versions available. Standard grade is the one to specify unless the drawing says otherwise; a low temperature grade is a different polymer balance and is quoted as a change of compound, not a change of supplier. FDA grades to 21 CFR 177.2600 are available on request.
Viton is a trade name of Chemours, and drawings still carry it. We quote the generic FKM designation and state the grade on the quotation, so a buyer comparing two suppliers compares polymer with polymer rather than brand with brand.
Sizes And Standards
Choosing between compounds rather than specifying one? The O-ring material comparison puts all five side by side at 70 Shore A, with the temperature range and the media each one cannot take.
The size is a separate decision from the compound, and it is the one buyers most often get wrong. The four standard lists are on their own pages, each with a lookup that takes either the code or a pair of measured dimensions: AS568 (inch dash numbers), ISO 3601 (Class A and Class B metric), JIS B 2401 (P, G, S, SS and V series) and BS 1806 (British imperial numbers). If the drawing gives a size outside those lists, or a cord that is not standard, we mould to drawing.
What To Send With An Enquiry
- The size or dash number, and the standard it comes from
- The medium, including any aromatic content, and the concentration for acids
- The maximum temperature and the minimum start-up temperature
- Hardness, and whether the seal runs dynamic
- Whether a specific grade, such as a low temperature or FDA compound, is written on the drawing
Is FKM the same as Viton?
Viton is one manufacturer’s trade name for FKM. The polymer family is the same, and the grade within it is what determines temperature and fluid behaviour, so a quotation should name the grade rather than only the brand.
What is the lowest temperature for FKM?
About −20 °C for a standard grade and −40 °C for a low temperature grade. Below that the ring takes a set and will not follow the groove on start-up, even if it seals once warm.
Will FKM seal steam?
Not for long. Hot water and steam attack fluoroelastomers, and the failure looks like a hardened, cracked ring rather than a swollen one. EPDM is the compound for steam.
Why is FKM so much more expensive?
The monomer cost. Fluorine content is bought by the kilogram and the curing chemistry is more involved, so the compound price is several times an NBR one. On a large static joint that cost is hard to justify; on a hot fuel line it is the only thing that works.